Storage Ring Input Coupler History
Sector |
Cavity | Ceramic Mfr.. | Coupler# |
Status (5+ kW Service) |
| Sector 36 | Cav1 | 1 - Failed - Ceramic Pinhole Leak | ||
MTM-22 |
2 - Current (34,648 hr.) as of 3/31/01 {INSTALLED 9/14/95} | |||
* |
Cav2 | MTM-06 | 1 - Failed - Ceramic Pinhole Leak | |
| MTM-20 | 2 - Failed - Ceramic Pinhole Leak | |||
| MTM-03 | 3 - Overheated - Copper Coated Ceramic | |||
| MTM-07 | 4 - Overheated - Copper Coated Ceramic | |||
| MTM-03 | 5 - Inoperable - Copper Coated Ceramic | |||
| ANL-01 | 6 - Overheated - Copper Coated Ceramic | |||
ANL-02 |
7 - Current (17,329 hr.) as of 3/31/01 {INSTALLED 12/15/98} | |||
| Cav3 | MTM-13 |
1 - Original (34,649 hr.) as of 3/31/01 {INSTALLED 2/15/95} | ||
| Cav4 | MTM-10 |
1 - Original (34,649 hr.) as of 3/31/01 {INSTALLED 2/5/95} | ||
| Sector 37 | Cav1 | MTM-14 |
1 - Original (24,000 hr.) - Overheating-Copper Coated Ceramic | |
ANL-06 |
2- (no probe) Overheating-Copper Coated Ceramic | |||
| Alborox | ANL-09 | 3 - Current (0 hr.) as of 3/31/01 {INSTALLED 4/2/01} | ||
* |
Cav2 | MTM-17 |
1 - Original (24,000 hr.) - Overheating-Copper Coated Ceramic | |
| Alborox | ANL-07** |
2 - Current (1,986 hr.) as of 3/31/01 {INSTALLED 12/26/00} | ||
| Cav3 | MTM-19 | 1 - Removed - Discolored Ceramic, but Functional | ||
MTM-15 |
2 - Current (30,587 hr.) {INSTALLED11/03/96} | |||
| Cav4 | MTM-15 | 1 - Removed - Galled Contact Ring Screws | ||
MTM-18 |
2 - Removed (23,000 hr.) Severe arcing on rear contact ring. | |||
| Alborox | ANL-08 |
3 - Current (2018 hr.) as of 3/31/01 (no probe) {INSTALLED 12/26/00} | ||
| Sector 38 | Cav1 | MTM-11 |
1 - Original (34,0792 hr.) as of 3/31/01 {INSTALLED 2/7/95} | |
* |
Cav2 | MTM-16 | 1 - Failed - Copper Coated Ceramic | |
| MTM-08 | 2 - Failed - Cracked Copper Coated Ceramic | |||
| MTM-07 | 3 - Overheated - Copper Coated Ceramic | |||
MTM-05 |
4 - Current (25,251 hr.) as of 3/31/01(re- cleaned){INSTALLED10/02/97} | |||
| Cav3 | MTM-09 |
1 - Original (34,793 hr.) as of 3/31/01 {INSTALLED 2/07/95} | ||
| Cav4 | MTM-12 |
1 - Original (34,793 hr.) as of 3/31/01 {INSTALLED 2/07/95} | ||
| Sector 40 | Cav1 | MTM-01 | 1 - Failed - Leaking Window Braze | |
MTM-21 |
2 - Current (34,604 hr.) as of 3/31/01 {INSTALLED 8/16/95} | |||
| Cav2 | MTM-02 | 1 - Damaged - Burnt Contact Ring | ||
| ANL-03 | 2 - Damaged - Copper Coated Ceramic (7,000 hr.) | |||
| Alborox | ANL-04 |
3 - Current (3,559 HR.) as of 3/31/01 {INSTALLED 10/02/00} | ||
* |
Cav3 | MTM-05 | 1 - Overheated - Copper Coated Ceramic | |
MTM-19 |
2 - Current (29,456 hr.) as of 3/31/01 {INSTALLED 1/30/97} | |||
| Cav4 |
Alborox |
MTM-04 |
1 - Original (34,604 hr.) as of 3/31/01 {INSTALLED 9/14/95} |
- * - BM Synchrotron X-ray Fan Location
- ** - Modified e-probe feed through per J. Jones
- XXX-XX - Current coupler
![]()
Please e-mail your comments to sharma@aps.anl.gov